Quote:
Originally Posted by walfreyydo View Post
Thanks for sharing.

My understanding is that these tubular manifolds are constructed of 321 stainless and require 347 filler rod or wire, as well as back-purging (because its stainless). If this is not done, it will just crack again.

I am curious when you mig welded this, if you used the above filler and back purging?

How long ago did you weld it and how has it held up?
i used 316L wire with Argon/Carbon Dioxide gas- shot blasted crack surface. Nothing out of the ordinary on the weld. It has been a few months and no issues yet- I'll post again if it fails.